Stress-optic coefficient 2026-11-05
The stress-optic coefficient measures the birefringence induced per unit principal-stress difference in the linear stress-optic law:
Here is a difference of refractive indices, so has SI units . The wavelength matters: a coefficient determined with one illumination wavelength should not simply be reused with another. The signs of and also require a consistent ordering of the optical axes and stresses.[ref]
For a uniform specimen of thickness viewed along a principal optical direction, the measured phase retardation is
A known uniaxial load supplies away from grips and other stress concentrations. Fitting the slope gives
Subtracting the unloaded retardation removes a constant background, but a load-dependent background must be investigated rather than absorbed into the coefficient.
For an original illustrative measurement, let , and produce . Then
Doubling the stress difference doubles the retardation only within the same linear regime. This numerical value is illustrative, not a material specification.
An equivalent magnitude convention uses the photoelastic fringe value . One additional full retardation cycle corresponds to for the uniform model. A fringe magnitude alone does not determine the sign of or the separate principal stresses.
The Illinois primary apparatus description makes the measurement chain concrete: a leadscrew loads the specimen, a load cell measures force, monochromatic light passes through the specimen between polarizing elements, and a camera records fringes. Establishing connects those optical observations to a mechanical stress scale. Wavelength, thickness, unloaded birefringence and loading conditions belong with the reported coefficient.[ref]
Stress-optic law 2026-11-05
The stress-optic law relates stress-induced birefringence to a mechanical stress difference. For an initially optically isotropic material in a suitable linear regime,
where are the principal stresses normal to the light path and is the stress-optic coefficient. Its units are , and its wavelength dependence matters when comparing optical measurements.[ref]
For uniform thickness and uniform relevant stress directions along the path, the measured phase retardation is
The measurement determines a difference, not both stresses separately. States and have the same difference and therefore the same retardation in this model. Extra mechanical information is needed to separate their absolute stress components.
A uniaxial calibration specimen gives a practical coefficient measurement. With axial force , known sectional area and negligible transverse stress, . If retardation plotted against force has slope , then
For illustrative , , and , this gives . A load would give stress difference and radians retardation. These are chosen calibration numbers, not a universal coefficient for a plastic.
A polariscope with controlled loading, a force readout and polarization analysis supplies the relevant apparatus.[ref] Background birefringence, thickness, temperature and wavelength should be accounted for. A measured intensity alone can have multiple compatible phase delays, and a changing optical-axis direction through a three-dimensional specimen can invalidate the simple scalar-path formula. The law is most useful when its optical and mechanical assumptions are checked together.
Waveplate 2026-10-14
A waveplate uses birefringence to change polarization of an electromagnetic wave through phase retardation. Its fast axis has the smaller refractive index, hence the larger phase velocity; its slow axis has the larger index. Consider normal incidence with the optic axis in the plate face, so both components follow the same straight path. A linear polarization at to these axes excites equal wave amplitudes.
A complementary experiment uses two sheet polarizers with a cellophane sheet between them. First cross the polarizers and remove the sheet: the field is dark. Insert and rotate the sheet about the beam: light returns at intermediate orientations, but extinction recurs at two perpendicular orientations. The sheet has changed the polarization of an electromagnetic wave, without requiring a resolved double image. With white light, different wavelengths can produce different transmitted colors.[ref]. Brightness alone does not establish circular polarization: an ideal rotating linear polarizer also gives orientation-independent light intensity for unpolarized light.