Convert atomic fractions to mass fractions before using the diagram's weight-percent scale:
With and , the overall is Sn. At , the diagram gives approximately and . These are about and Sn. The lever rule gives
The microstructure has primary Bi-rich crystals surrounded by remaining liquid. The phase compositions and fractions are approximate readings of a printed phase diagram, not exact thermodynamic values. Faster cooling generally gives finer crystals, solute segregation and departure from these equilibrium compositions.
At , the stable sequence is , , . The stable two-solid common tangent lies below the liquid curve. There is no stable liquid interval, although a metastable extrapolated liquid Gibbs free energy can still be drawn.
Figure 1.
Qualitative Gibbs free-energy envelopes above, at and below a binary eutectic
. Original illustrative curves with constructed tangencies. Free-energy units and curvatures are arbitrary, not measured thermodynamic data for bismuth-tin. Details.
At , one line is tangent to all three Gibbs free energy curves at approximately for (Bi), for liquid, and for . These three phases can coexist at the eutectic point. Between the two solid compositions, the equilibrium phase fractions depend on how much liquid has already transformed; exactly at the invariant temperature, the overall composition alone does not fix all three fractions. At the eutectic overall composition, cooling just below the temperature eliminates the liquid and leaves the two solids.
At , moving from Bi-rich to Sn-rich composition gives , , , , . Approximate liquid coexistence compositions read from the diagram are on the left and on the right; the coexisting solids lie near their respective pure ends. The stable Gibbs free energy follows solid curves near the endpoints, two common-tangent constructions in the coexistence intervals, and the liquid curve between them.
The first peak is , with ; the second is , with . Applying Bragg's law with gives
Thus , consistent with the approximate ratio used to order the reflections. These are the lengths of the supplied larger basal cell; the primitive basal lattice parameter is .
Ordering reflections by with , the first three nonzero families are , and . The family is extinct. Their structure factors are
The atomic scattering factors in each expression are evaluated at that reflection's scattering vector, so equal symbolic forms need not mean equal numerical amplitudes at different angles. In particular, the low-angle superlattice peaks need not be the strongest peaks.
Summing phase-weighted atomic scattering factors over the four positions gives
If have different parity, the reflection vanishes. If they have equal parity, this becomes . The difference reflections reveal chemical order; they disappear when all sites instead have the same average scattering factor.
Barium titanate has a high-temperature cubic perovskite structure, with Ti centred in its oxygen octahedron on average. This phase is paraelectric. Near room temperature the structure is tetragonal, with relative ionic displacements that give a spontaneous electric polarization. This phase is ferroelectric: an applied electric field can switch between differently polarized domains. Both phases have the same composition, BaTiO; the transition near changes crystal symmetry and electrical response.
In crystal polymorphism, the same chemical composition has different crystal structures; for an chemical element, this is a form of allotropy. Diamond has a three-dimensional tetrahedral network of covalent bonds, giving high hardness and a wide band gap. Graphite has strongly bonded planar sheets, with weaker interactions between sheets. Sliding between sheets makes it a useful solid lubricant; mobile electronic states give good electrical conduction within the sheets. Their different properties come from different bonding and structures, despite both being carbon.
The conventional relaxation-loss peak near applies to fixed strain amplitude, not to fixed stress amplitude. This distinction matters because the question explicitly describes oscillating stress.
The full complex modulus of the series Maxwell element is
For imposed strain , the energy dissipated per volume per cycle is
Since has its maximum at , fixed-strain loss per cycle peaks at . At that scale the imposed cycle time is comparable with the relaxation time, and substantial viscous flow occurs while stress remains appreciable.
For the literally stated comparison with fixed stress amplitude, use the compliance
The dashpot strain rate is . Its dissipation integrated over a period gives
This decreases monotonically with frequency; there is no finite-frequency maximum at fixed stress amplitude in the ideal Maxwell model. Its mean dissipated power is , independent of frequency. The formal low-frequency divergence in energy per cycle accompanies very large strain excursions and cannot be extrapolated beyond the linear model's range. The graph identifies both results rather than assigning the fixed-strain peak to the wrong loading condition.
With , the curve is
It rises linearly from zero, bends downward and approaches the plateau . Its half-height occurs at .
For , the dashpot contributes the larger strain and dominates the compliant response. For , dashpot deformation during a cycle is small relative to spring strain, and the response is spring-dominated. The crossover separates these regimes rather than a discontinuous transition.
Figure 1.
Original Maxwell storage curves versus squared frequency and the distinct dissipation laws at fixed strain and fixed stress amplitudes; axes use logarithmic spacing to show both regimes
. Details.
For high-strength steel, use
At fixed toughness, raising yield stress reduces quadratically but reduces the required pressure thickness only linearly. Thus a higher-strength grade can have a worse leak-before-break screening margin. The relevant screening combination is , since simultaneous satisfaction requires
Use measured low-temperature toughness and appropriate joining/environmental performance; strength alone does not establish suitability. The comparison also has to remain within the thin-wall approximation.
TODO: numerical thickness cannot be completed without the unavailable 2018 NST Data Book's high-strength-steel property pair. The four material rankings cannot be made numerically definitive from the exam PDF alone.
For mild steel, the corresponding bounds are
A relatively low yield stress increases the thickness needed to carry pressure, but a favorable toughness-to-yield-strength ratio can give a much larger leak-before-break upper bound. This tradeoff often makes a tough structural steel more attractive than choosing the highest strength alone.
For Arctic service, the ductile-to-brittle transition is crucial. A room-temperature toughness cannot be assumed to persist below the transition, and welding, constraint and loading rate affect the comparison. A suitably qualified low-temperature steel can be practical; the word mild alone does not establish that qualification.
TODO: numerical thickness cannot be completed without the unavailable 2018 NST Data Book values. The temperature and state of the tabulated toughness must also be identified before making a numerical service claim.
For Ti–6Al–4V, use its own fracture toughness and yield stress in
The same unit-conversion formulas from part(i) apply. A feasible yield-limited screening interval requires , using consistent crack geometry and low-temperature properties.
High specific strength and corrosion resistance can be attractive, but cost, fabrication, joining and toughness must also be assessed. The label HCP is not a sufficient rule that every titanium alloy has the same sharp ductile-to-brittle transition as ferritic steel; actual low-temperature alloy and microstructural data are needed.
TODO: numerical thickness cannot be completed without the unavailable 2018 NST Data Book's Ti–6Al–4V property pair. No historical value or material-specific Arctic toughness is invented.
For the aluminium alloy, write and for the appropriate data-book properties at the relevant material state and temperature. The yield-limited screening bounds from part(c), with , are
For in and in , the numerical substitutions are and .
A high-strength alloy's large yield stress can require a small allowable leak-before-break thickness even when its minimum pressure thickness is modest. FCC structure generally favors low-temperature plasticity, but does not by itself establish the alloy's fracture toughness, weld performance, corrosion behavior or fatigue resistance.
TODO: numerical thickness cannot be completed without the 2018 NST Data Book values and alloy condition, which are unavailable. The accessible Engineering2011/revised2019 book is not confirmed as the supplied edition; generic aluminium property ranges are not substituted as if they were the exam's values.
Ferrite etches faster in Nital, so it recedes and leaves cementite standing as the higher ridges. The identification is based on the surface-relief preparation, not on assuming that every bright feature in every microscopy mode is cementite. In the stated AFM image, brightness is a displayed height contrast.
The profile estimate and equilibrium lever-rule estimate need not agree exactly. The height trace contains only four major ridges, making it a small sample of the microstructure. Pixel size, ridge-threshold choice, tip geometry, contamination, polishing damage and unequal etching change apparent widths. A finite-radius AFM tip can broaden the narrow raised cementite regions, biasing their inferred fraction upward.
The equilibrium calculation assumes eutectoid pearlite with the chosen carbon composition and tie-line values. Off-eutectoid steel can include proeutectoid ferrite or cementite outside the pearlite; alloying, carbon segregation and non-equilibrium cooling alter the simple Fe–C estimate. Carbon solubility also varies with temperature. The mass-to-volume conversion requires phase densities.
The observed difference between roughly ridge fraction and equilibrium phase volume is therefore a reason to examine sampling and the etched-surface measurement, not to force the image widths to match the lever rule. Multiple colonies, repeated calibrated traces and a phase-sensitive measurement would improve the comparison.

There are unlisted articles, also show them or only show them.